Restaurări protetice pe suport din zirconiu placate cu mase ceramice în edentația frontală
Zirconia-based prosthetic restorations veneered with ceramic materials for the rehabilitation of anterior edentulous spaces
Data primire articol: 23 Octombrie 2026
Data acceptare articol: 30 Octombrie 2026
Editorial Group: MEDICHUB MEDIA
10.26416/ORL.73.4.2026
Descarcă pdf
Abstract
Zirconia-based prosthetic restorations veneered with ceramic materials have been extensively studied over time, becoming the ideal solution today for rehabilitating anterior tooth loss. Given that zirconium oxide is a biomaterial with a relatively short history, research into it remains ongoing. Therefore, this article presents the use of zirconium oxide in the manufacturing of prosthetic restorations for anterior edentulous spaces.
Keywords
prosthetic restorationszirconiaanterior edentulous spacesRezumat
Restaurările protetice pe infrastructuri din zirconiu placate cu mase ceramice au fost cercetate în foarte mare detaliu de-a lungul timpului, devenind astăzi soluția ideală în reabilitările de edentație frontală. Întrucât oxidul de zirconiu este un biomaterial cu istoric relativ scurt, cercetările asupra acestuia continuă și în prezent. Astfel, în acest material vom prezenta utilizările oxidului de zirconiu în confecționarea restaurărilor protetice în edentația frontală.
Cuvinte Cheie
restaurări proteticezirconiuedentație frontalăIntroduction
From ancient times to the present day, numerous studies have demonstrated that individuals who smile naturally and confidently, with harmonious facial symmetry, report a higher quality of life than those who avoid smiling because of dental conditions affecting both esthetics and function. Moreover, the simple act of smiling positively influences not only the individual but also those around them by promoting a positive emotional state, an aspect that is often underestimated regardless of the type of activity undertaken(1-5).
General considerations
In general, the primary focal elements of a smile are the anterior teeth, namely the central incisors, lateral incisors and canines, located in both the maxillary and mandibular arches. Their position, degree of rotation, inclination and characteristic crown morphology collectively determine the overall appearance of the smile(1-5).
More specifically, the position and morphology of the anterior teeth within the prosthetic field are of particular importance in establishing the occlusal relationship between the two dental arches while simultaneously contributing to facial esthetics. When anterior edentulism occurs – that is, the absence of teeth belonging to the maxillary and/or mandibular anterior segments –, the consequences extend beyond esthetic concerns and diminished self-confidence resulting from reluctance to smile or speak openly. These defects also produce significant functional impairments. In addition to severely affecting facial appearance, anterior edentulous spaces, whether maxillary, mandibular, or involving both arches, compromise essential mandibular movements, including protrusive movements and canine-guided lateral excursions. Furthermore, mastication and phonation are adversely affected, potentially leading to broader consequences involving the digestive system, the temporomandibular joint, and the associated musculature. Consequently, the prosthetic rehabilitation of anterior edentulism represents one of the most demanding clinical challenges encountered by the dental team, requiring close collaboration between the dentist and the dental technician(1-5).
This paper aims to present both general and specific technological aspects involved in the CAD/CAM fabrication of zirconia-based prosthetic restorations veneered with ceramic materials for the functional rehabilitation of anterior edentulous spaces.
Case presentations
Case 1: Rehabilitation of tooth 1.2 edentulism
A 36-year-old patient presented to the dental clinic for the prosthetic rehabilitation of a missing maxillary lateral incisor (tooth 1.2). Following clinical and radiographic examination, the dentist and patient jointly decided on an implant-supported prosthetic restoration. A Megagen dental implant was placed, and the subsequent implant-prosthetic rehabilitation was performed using the corresponding implant system and its dedicated components.
Initially, the dentist made an impression of the arch requiring rehabilitation using double-mix addition silicone impression material (putty and light-body consistency) in a standard impression tray to obtain maximum accuracy in the implant area. The opposing arch was impressed using putty condensation silicone in a standard tray. Both impressions were rinsed under tap water for 15 seconds and subsequently decontaminated by immersion in a disinfectant solution containing quaternary ammonium compounds, strictly following the manufacturer’s recommendations.
The definitive impression obtained with double-mix addition silicone served as the basis for positioning the implant analog, thereby accurately reproducing the implant position present in the oral cavity.
The implant analog was secured using the dedicated Megagen driver. The impression was again rinsed and disinfected according to the previously described protocol (Figure 1).
/art%205/Figure%201.%20Opposing%20arch%20impres.jpg)
The definitive impression was then isolated using a specialized separator to facilitate the subsequent application of artificial gingiva. A rigid addition silicone material was applied around the implant analog to reproduce the peri-implant soft tissues. The separator ensured that, following removal of the impression, the artificial gingiva remained attached to the working cast (Figure 2).
/art%205/Figure%202.%20Applying%20the%20separat.jpg)
The next stage consisted of manufacturing working cast from type IV dental stone. In this case, the models were not physically mounted in an articulator because the patient’s occlusal relationship was stable, and the lateral incisor was designed to remain out of occlusion, consistent with the adjacent anterior teeth. After trimming, the casts were prepared for scanning.
A scan body compatible with the implant system was used to design a customized abutment that would support the zirconia-based crown. The scan body, which was also compatible with the laboratory scanner, accurately reproduced the implant position and was attached with its reference window facing the buccal aspect. The laboratory scanner sequentially captured the working cast, the opposing cast and the interocclusal relationship. These digital data were transferred to the CAD software, where both the customized abutment and the definitive crown were designed (Figure 3).
/art%205/Figure%203.%20Maxillary%20working%20ca.jpg)
Using the CAD software, the zirconia framework for the future restoration was designed according to its appropriate position within the dental arch. The software eliminated unnecessary scanned areas and identified regions of interest that were not readily visible. Within the CAD environment, the precise implant position and the cervical finish line of the zirconia framework were established before designing the coping itself. A tooth morphology closely matching the adjacent dentition was selected from the software library as the initial template.
The coping was subsequently reduced to provide approximately 2 mm of space for ceramic veneering during the final laboratory stage. All margins and internal angles were rounded to minimize the risk of ceramic microfractures. The completed design was then transferred to the CAM milling unit, which milled the three-dimensional framework from a pre-sintered zirconia disc using dedicated milling burs. The milled framework was intentionally oversized to compensate for sintering shrinkage; after sintering, it reached the planned final dimensions (Figure 4).
/art%205/Figure%204.%20Zirconia%20coping%20on%20t.jpg)
Following sintering, a ceramic veneering material specifically developed for zirconia frameworks (VITA zirconia ceramic system) was applied by brush technique. The restoration underwent a single firing cycle during which the dentin layer was applied first, followed by the enamel layer in the incisal third. The crown was subsequently refined using diamond burs and discs to create an appropriate surface texture for optimal ceramic integration. Finally, a glaze layer was applied, providing the definitive shade and translucency that closely resembled natural dental tissues. The completed implant-supported zirconia crown veneered with ceramic was cemented onto the customized implant abutment. The cement space had been predetermined during the CAD design phase at 0.4 mm. Consequently, this clinical case combined both a digital CAD/CAM workflow and essential conventional laboratory procedures (Figure 5).
/art%205/Figure%205.%20Implant-supported%20pr.jpg)
*
Case 2: Prosthetic rehabilitation of the entire maxillary anterior segment using a fixed dental bridge and single crowns
A 47-year-old female patient presented to the dental clinic for the prosthetic rehabilitation of a maxillary anterior edentulous space. Following clinical and radiographic examination, the dentist and patient jointly established a treatment plan consisting of a fixed dental bridge supported by teeth 1.1 and 2.3, together with single crowns on teeth 1.2 and 2.2. Several dental implants had previously been placed in the posterior region; however, this report focuses exclusively on the prosthetic rehabilitation of the anterior region. All anterior restorations were highly esthetic zirconia-based restorations veneered with ceramic materials.
The initial clinical stage involved making a preliminary impression of the maxillary prosthetic field using a standard impression tray and an irreversible hydrocolloid (alginate) impression material. After decontaminating the impression and pouring the preliminary cast, the dental technician fabricated an individualized impression tray using light-cured composite resin.
Using this custom tray, the dentist obtained the definitive impression with addition silicone impression materials, which served for the fabrication of the working cast. During the preliminary impression stage, an impression of the opposing dental arch was also obtained using a standard tray and condensation silicone putty. At the same appointment, the intermaxillary occlusal relationship was recorded using a condensation silicone bite registration material. The preliminary impression, definitive impression and opposing arch impression were all rinsed under running water for approximately 15 seconds before being disinfected by immersion in a quaternary ammonium compound solution, strictly according to the manufacturers’ recommendations.
The working cast and opposing cast were then fabricated using type IV dental stone. In this case, the working cast was produced using the Giroform casting system. Areas containing undercuts or retentive features that could interfere with the insertion of the future restorations were blocked out with a specialized wax. After cast preparation, the models were positioned according to the recorded occlusal relationship and mounted in an articulator following standard mounting procedures. The casts were stabilized using transparent silicone material applied bilaterally.
To fabricate the zirconia framework, the working cast, opposing cast, prepared abutments and the articulator-mounted assembly were prepared for the scanning and CAD design stages, with unnecessary areas removed beforehand. The zirconia framework was designed using the CAD system, while the CAM milling unit transformed the digital design into the physical restoration (Figure 6).
/art%205/Figure%206.%20Maxillary%20definitive.jpg)
Within the CAD software, the cervical finish line was established, the insertion path was selected, and a tooth morphology was chosen from the software library to harmonize with the existing dentition. The connector dimensions between the pontics and abutment teeth were carefully designed, while the zirconia copings were reduced to provide sufficient space for ceramic veneering. Cement space was defined, and all restoration surfaces were smoothed before the design was finalized.
The completed digital design was transferred to the CAM milling unit, where milling was performed under dry conditions using pre-sintered zirconia discs. As expected, the milled framework was intentionally oversized and subsequently achieved its planned dimensions after sintering. Following sintering, the zirconia framework was cleaned with a steam cleaner and prepared for ceramic application (Figure 7).
/art%205/Figure%207.%20Zirconia%20frameworks.jpg)
For this case, Noritake ceramic specifically designed for zirconia frameworks was selected. The ceramic powder was mixed with distilled water to obtain the appropriate consistency and applied using a brush technique. Shade A3, corresponding to the Vita shade guide, was selected.
The pink ceramic simulated dentin, whereas the blue ceramic reproduced enamel characteristics. Ceramic was applied incrementally, layer by layer, until the desired tooth morphology was achieved.
After the dentin layer was completed, the enamel layer was applied, primarily in the incisal region and, to a lesser extent, on the proximal surfaces, while dentin covered the entire zirconia framework.
The isolated cast was covered with a moistened tissue strip adapted to the contour of the edentulous ridge, allowing accurate reproduction of the gingival contact area beneath the pontics. The tissue strip facilitated removal of the ceramic restoration from the cast without distortion.
Once the desired morphology had been achieved, the veneered zirconia framework was removed from the cast, positioned on firing pins, and placed in the ceramic furnace. After each firing cycle, the ceramic surface was refined before the subsequent firing. Following the application of the final ceramic layer, a glaze layer was applied (Figure 8).
/art%205/Figure%208.%20Ceramic%20materials%20us.jpg)
*
Case 3: Rehabilitation of the maxillary anterior segment using zirconia copings veneered with ceramic materials
A 33-year-old male patient presented for prosthetic rehabilitation of the entire maxillary anterior segment, as all anterior teeth were affected by extensive carious lesions. Following clinical and radiographic examination, the dentist and patient agreed on a treatment plan consisting of six highly esthetic individual zirconia-supported crowns veneered with ceramic materials.
Initially, a definitive maxillary impression was obtained using a standard tray and double-mix addition silicone material. The impression was subsequently rinsed and disinfected according to established clinical protocols, after which the working cast was fabricated using the Giroform system.
Once the dental technician obtained the maxillary working cast and mandibular opposing cast, the prepared abutments were sectioned and engraved. Sectioning was performed with a diamond disc, while engraving was completed using tapered burs. Before scanning, each prepared abutment was carefully evaluated.
A thin layer of wax was applied to smooth rough surfaces and facilitate scanning. The laboratory scanner produced significantly clearer digital images after the application of corrective wax or light-colored scanning spray, thereby reducing the need for rescanning (Figure 9).
/art%205/Figure%209.%20Impression%20of%20the%20de.jpg)
Each component was subsequently scanned individually according to the sequence indicated by the scanner software. After scanning the working cast, opposing cast, removable dies and occlusal relationship, unnecessary scanned areas were eliminated and the digital information was transferred to the CAD software.
Once the patient information had been entered, the CAD software required specification of the restoration type, number of restorations, working area, opposing dentition, and selected material, in this case, zirconium oxide. The software offered an automatic design proposal while allowing the dental technician to perform manual modifications whenever necessary.
The cervical finish line was established by placing reference points along the highest cervical margins. After determining the insertion path, the technician selected the appropriate tooth morphology from the virtual library. The zirconia copings were reduced to create the necessary support thickness, while the final anatomical form would subsequently be achieved through ceramic veneering.
Special attention was paid to preserving proper contact points, eliminating sharp edges and angles, verifying adequate space for ceramic application, and aligning the incisal edges as closely as possible.
After completing the CAD design, the digital data were transferred to the CAM milling unit. A highly translucent D2-shade zirconia disc was selected. The restorations were milled from a pre-sintered zirconia disc, resulting in oversized copings that compensated for sintering shrinkage.
The copings were then positioned in sintering supports, and the appropriate sintering program was initiated. Upon completion of the process, the restorations achieved their intended dimensions and mechanical strength (Figure 10).
/art%205/Figure%2010.%20Initial%20stages%20of%20c.jpg)
The zirconia frameworks were subsequently prepared for the application of the external ceramic veneer. This procedure provided the restorations with the desired esthetic characteristics while preserving the mechanical advantages of zirconia.
The ceramic material was applied with great precision using brushes of various sizes. The final glaze application represented the last laboratory stage, giving the restorations their natural appearance, surface luster and esthetic integration.
Ultimately, the zirconia-based restorations acquired the color and appearance of natural teeth through ceramic veneering. The combination of zirconia’s mechanical strength and the superior esthetics of dental ceramics makes these restorations an excellent option for anterior prosthetic rehabilitation (Figure 11).
/art%205/Figure%2011.%20Zirconia%20frameworks.jpg)
Discussion
The use of zirconium dioxide as a substrate for prosthetic restorations has evolved from an exotic procedure into a sustainable and widely accessible one(6,7). This evolution, driven primarily by its mechanical and optical properties, has led practitioners to increasingly recommend zirconium dioxide over metal-ceramic restorations(8,9).
The opacity of zirconium dioxide, combined with a color resembling natural tooth structure, makes this material a suitable choice regardless of the underlying support. Whether used for restorations on natural teeth or implants, zirconium oxide-based restorations offer an optimal balance between the strength required for mastication and patient esthetic expectations, irrespective of their position within the dental arches(10,11).
Another important aspect is that the use of zirconium dioxide involves digital workflows, which reduces the error rate. Cast analysis allows for much more accurate visualization, and the use of a comprehensive algorithm based on thousands of models enables the creation of a form that is far superior in terms of both esthetics and function(12,13). However, the esthetic aspect remains the responsibility of the dental technician who, based on accumulated experience, achieves a perfect balance between patient requirements and the limitations imposed by the materials(14,15).
Conclusions
Zirconia-based prosthetic restorations veneered with ceramic materials have been extensively investigated over time and have become one of the preferred solutions for the rehabilitation of anterior edentulous spaces. Because zirconium oxide is a biomaterial with a relatively short clinical history, research into its properties and applications continues to evolve. At the same time, dental ceramics have undergone remarkable development, significantly improving the esthetic outcomes of oral prosthetic rehabilitation.
The evidence presented in this paper suggests that the combination of zirconia frameworks and veneering ceramics successfully integrates high mechanical strength with excellent esthetics, making it particularly suitable for the prosthetic rehabilitation of anterior edentulous regions.
Furthermore, advances in CAD/CAM technology have enabled the precise fabrication of zirconia-based restorations veneered with ceramic materials. Whether applied to implant-supported abutments, natural tooth preparations or fixed dental bridges, these restorations represent reliable treatment options for the anterior region. Given the high esthetic demands associated with this area, the combination of zirconia and veneering ceramics successfully fulfills both functional and esthetic clinical requirements.
Conflict of interests: none declared.
Financial support: none declared.
This work is permanently accessible online free of charge and published under the CC-BY.
Corresponding author: s: Viorel Ștefan Perieanu E-mail: viorel.perieanu@umfcd.ro; Ioana Voinescu E-mail: ioana.voinescu@umfcd.ro
Bibliografie
- Moskowitz ME, Nayyar A. Determinants of dental esthetics: a rational for smile analysis and treatment. Compend Contin Educ Dent. 1995;16(12):1164-1186.
- Rosenstiel SF, Land MF, Fujimoto J. Contemporary fixed prosthodontics, 3rd Edition. Mosby St. Louis, 2001.
- Bratu D, Nussbaum R. Bazele clinice și tehnice ale protezării fixe. Editura Helicon, Timișoara, 2001.
- Moldoveanu DLE. Tehnologia protezelor unidentare. Caiet de lucrări practice. Ovidius University Press, 2012.
- Bayne SC. Dental restorations for oral rehabilitation – testing of laboratory properties versus clinical performance for clinical decision making. J Oral Rehabil. 2007;34(12):921-932.
- Takeichi T, Katsoulis J, Blatz MB. Clinical outcome of single porcelain-fused-to-zirconium dioxide crowns: A systematic review. J Prosthet Dent. 2013;110(6):455-461.
- Schneebeli E, Brägger U, Scherrer SS, Keller A, Wittneben JG, Hicklin SP. Quality Evaluation of Zirconium Dioxide Frameworks Produced in Five Dental Laboratories from Different Countries. J Prosthodont. 2017;26(5):399-409.
- Zhang Y, Lawn BR. Evaluating dental zirconia. Dent Mater. 2019;35(1):15-23.
- Larsson C. Zirconium dioxide based dental restorations. Studies on clinical performance and fracture behaviour. Swed Dent J Suppl. 2011;(213):9-84.
- Shihabi S, Chrcanovic BR. Clinical outcomes of tooth-supported monolithic zirconia vs. porcelain-veneered zirconia fixed dental prosthesis, with an additional focus on the cement type: a systematic review and meta-analysis. Clin Oral Investig. 2023;27(10):5755-5769.
- Raigrodski AJ, Yu A, Chiche GJ, Hochstedler JL, Mancl LA, Mohamed SE. Clinical efficacy of veneered zirconium dioxide-based posterior partial fixed dental prostheses: Five-year results. J Prosthet Dent. 2012;108(4):214-22.
- Dyakonenko EE, Sakhabieva DA, Axelrod IB, Lebedenko IY. Sravnitel’naya otsenka traditsionnogo i skorostnogo obzhiga stomatologicheskoi keramiki na osnove dioksida tsirkoniya [Comparative evaluation of traditional and speed sintering of dental ceramics based on zirconium dioxide]. Stomatologiia (Mosk). 2022;101(2):106-113. Russian.
- Riedel C, Wendler M, Belli R, Petschelt A, Lohbauer U. In vitro lifetime of zirconium dioxide-based crowns veneered using Rapid Layer Technology. Eur J Oral Sci. 2019;127(2):179-186.
- Prause E, Hey J, Sterzenbach G, Beuer F, Adali U. Survival and success of veneered zirconia crowns. Int J Comput Dent. 2023;26(3):247-255.
- Alghauli M, Alqutaibi AY, Wille S, Kern M. 3D-printed versus conventionally milled zirconia for dental clinical applications: Trueness, precision, accuracy, biological and esthetic aspects. J Dent. 2024;144:104925.